Ok, so the experiment with the clay and perlite is finally finished. Perlite already contains a lot of alumina, so I tried just mixing clay with powdered perlite (I used the bottom of a metal cup to crush it; a better option would have been a ball mill). The first brick was even parts (by volume). It cracked into two pieces and had a lot of spalling. The second was 2 parts perlite to 1 of clay. It broke in two, with only a little spalling. The last was 3 parts perlite powder to 1 part clay. The surface melted slightly, but there was no cracking or spalling. (I believe the last brick was tested after I started using fuel pellets, so the temperature was probably considerably higher than with the first two.)
So, my plan was to line the next forge with the 3 to 1 mixture of perlite powder and clay. I was also going to add some non-powdered perlite, but only pieces between 1mm and 3mm. I ran into a problem with this. Powdering perlite takes a long time. Also, perlite is mostly air, which means that an 8 quart bag of perlite yields only about 2-3 cups of powder. So, I started looking around for alternative refractory mixtures again.
This time I found a mixture that looks really good. The recipe is 2 parts clay, 2 parts silica sand (beach sand is primarily silica; play sand at hardware stores is also mostly silica), 1.5 parts perlite, and 1.5 parts Portland cement. I used this mixture, but I added the 3-4 cups of powdered perlite to the mix, and I also increased the portion of regular perlite, to improve its insulating properties.
I have not tested this mixture with heat yet, but I have finished the forge and will be testing it once it is totally cured and dried.
Showing posts with label refractory. Show all posts
Showing posts with label refractory. Show all posts
Monday, January 31, 2011
Subscribe to:
Posts (Atom)